Wear rate of Zirconium Silicate beads in Lab
1. Typical Properties:
|
|
NaorZr-64 |
Fused one |
Sintered another one |
|
Specific Gravity(g/cm3) |
4.11 |
3.75 |
4.09 |
|
Hardness Vickers(Hv) |
1073.2±12.0 |
640.7±28.4 |
996.6±16.2 |
|
Crushing Strength(kgf) |
116.70±15.42 |
45.43±17.28 |
78.42±37.71 |
|
Microstructure |
zircon crystals |
zirconia crystals divided glassy phase |
zircon crystals with porosity |
2. Chemical Composition:
|
composition |
NaorZr-64 |
Fused one |
Sintered another one |
|
ZrO2 |
62-64% |
68% |
58% |
|
SiO2 |
33% |
31% |
37% |
3. Wear rate in laboratory:
A. Testing condition
Mill: vertical type
Volume of grinding container: 1.4L
Speed of shaft: 1500rpm
Length of pins: 90mm
Diameter of beads: 1.93±0.08mm (NanorZr-64),
1.89±0.10 mm (Fused one),
1.91±0.09mm (Sintered another one)
Charge of beads: 650ml
Grinding powder: 50g Al2O3 with 325 mesh particle sizes
Base: 450ml water
Grinding time: 8h
B. Wear rate (%):
|
NanorZr-64 |
Fused one |
Sintered another one |
|
1.3624 |
4.9276 |
3.6308 |